AISI 8620 (21NiCrMo2) welding procedure & guidelines

AISI 8620 Material

AISI 8620 steel is a low alloy-medium carbon steel, alloyed with Nickel, chromium and molybdenum used for application requires high strength and toughness. 8620 is used for gear & shaft are usually case hardened to provide improved wear resistance.

Due to higher carbon percentage with addition of austenitic stabilizers, AISI 8620 response very good to heat treatment which are mainly used for increasing the hardness of this alloy.

AISI 8620 welding guidelines

Chemical and mechanical properties of AISI 8620

The UNS number of AISI 8620 is G86200. The ASME P number for AISI 8620 is P No. 3, Group No. 3.

ASTM equivalent of AISI 8620 is ASTM A 108 grade material. This is a pressure grade bar material.

The carbon percentage of AISI 8620 is 0.18 to 0.23%, Nickel 0.4-0.6%, Chromium 0.4 to 0.6 & molybdenum 0.15 to 0.25%. AISI 8620 equivalent materials are 21NiCrMo2, 805M20 & SNCM220.

Yield strength of AISI 8620 is 385 N/mm2 (56Ksi) and tensile strength is 530 N/mm2 (77Ksi).

AISI 8620 vs 4140

AISI 8620 (ASTM A108) is an alloy of Ni, Cr & Mo with medium carbon range while AISI 4140 is a high carbon steel alloyed with Cr & Mo only.

There is no Nickel in AISI 4140 alike in AISI 8620. 4140 due to higher carbon percentage is mostly used in quenched & tempered (Q & T) conditions.

The chemical properties of AISI 4140 are given below for your comparison.

Carbon       Si     Mn       Cr       Mo        S      P
      0.40     0.30      0.88      1.10      0.24     0.015    0.021

Click to read: How to weld AISI 4140 Steel – www.materialwelding.com

Weldability of AISI 8620

AISI 8620 has moderate weldability and can be welded without much concerns when proper practices are implemented.

See also  Quality Control Inspection - Why it's Important

Welding of 8620 in annealed condition is much easier compared to welding in case hardened conditions. The welding electrode selection is based on the weld metal strength requirements.

Stick/ SMAW Welding of AISI 8620

Stick welding or SMAW welding of AISI 8620 is carried out using E9018-G or E9018-M (AWS SFA 5.5).

Before the welding, its essential to Preheat the base material to 350- 400ºF & interpass temperature shall be maintained to maximum 600 °F (315 °C).

Low hydrogen electrodes must be baked fully prior to use. Baking guidelines for low hydrogen electrodes are given in below link.

What is Low Hydrogen electrodes, Their Storage & Baking Procedure?

Post weld heat treatment (PWHT) if required shall be carried out at 1150 to 1200 ºF. Holding time is usually 1 hour per inch of the material thickness.

TIG and MIG Welding of AISI 8620 is done using ER90S-G type filler wire.

How to Weld AISI8620 to Mild Steel, A36 and A1018

Stick or SMAW Welding of AISI 8620 to mild steel grades or carbon steel grades such as ASTM A36, ASTM A106 Grade 1018 shall be carried out using E9018-G. E9018-M (AWS SFA 5.5).

E7018 type welding electrode can also be used for welding 8620 material with carbon steel without any problem.

Preheating is necessary only for 8620 material and no preheating is required for carbon steel material.

How to Weld AISI 8620 to AISI 4140

Click to read: How to weld AISI 4140 Steel

Stick Welding of AISI8620 to AISI 4140 can be done using E9018-G or ER90S-G type rod. Low hydrogen electrodes must be baked prior to use.

See also  How to weld T-1 ASTM A514, A517 Quenched & tempered grades

After welding, cover the welding with Kaowool to allow slow cooling and help to control the weld hardness.

How to Weldcase hardened 8620 steel

Welding of case hardened AISI 8620 require high care as the hardened area has high carbon and hard microstructure which is prone to weld cracking.

If welding is required, preheat the area to higher temperature around 500ºF and maintain the preheat during the welding process.

Use E9018-G electrode for welding. If crack persists, use E7018 type rod that is having softer weld metal compare to E9018-G rod. After welding, cover the part under Kaowool to allow slow cooling.


Material Welding is run by highly experienced welding engineers, welding trainers & ASNT NDT Level III bloggers. We strive to provide most accurate and practical knowledge in welding, metallurgy, NDT and Engineering domains.