Short Circuit Welding Transfer

What is Short circuit transfer in welding?

In short circuit transfer, the amperage used in relation to the wire size is low, causing the wire to melt at the electrode tip without detaching.

As the wire feeder continues to feed the wire, the molten electrode tip makes contact with the weld pool, causing the amperage to increase and the magnetic pinch effect to act on the electrode tip.

This results in the magnetic forces pinching off the droplet, which is then drawn into the weld pool by surface tension forces.

The gap between the electrode and the weld pool is then re-established, and the arc is re-established.

This process occurs rapidly, more than 100 times per second, making the short circuits imperceptible to the human eye and creating the illusion of a continuous arc.

What causes Short Circuit Welding?

Short circuit welding occurs when the welding wire comes into contact with the base metal, causing a momentary short circuit. This is also known as “short-circuit transfer” in GMAW (Gas Metal Arc Welding).

What is the difference between spray transfer and short circuit?

In MIG and MAG welding, the spray arc achieves the highest deposition rate. This enables the welder to weld medium and thick plates. 

Spray arcs are often used in gas-shielded arc welding for filler and cover passes. The spray arc can be ignited without a short circuit. The material transition is very fine droplets with low spatter formation.

FeatureSpray TransferShort Circuit Transfer
Heat inputHigh heat inputLow heat input
Welding speedHigh welding speedLow to medium welding speed
Welding positionFlat or horizontalAll positions (flat, horizontal, vertical, overhead)
Metal thicknessThick materials (over 1/8 inch)Thin to medium materials (up to 1/8 inch)
SpatterHigh spatterLow spatter
Shielding gas100% CO2 or mixed gas with high CO2 content100% CO2 or mixed gas with low CO2 content
Voltage and CurrentHigh voltage and currentLow voltage and current
PenetrationDeep penetrationShallow penetration
AppearanceRough, with a wider bead patternSmooth, with a narrow bead pattern
Skill level requiredAdvanced welding skills requiredBeginner to intermediate welding skills required

For Spray Transfer, a much higher voltage is needed to ensure that the wire does not make contact, ie short circuit, with the weld pool. 

See also  Overhead Welding tips and technique for Stick and MIG welding

The molten metal at the tip of the wire is transferred to the weld pool in the form of a spray of small droplets (smaller than the diameter of the wire). 

However, there is a minimum current level or threshold below which the drops will not be violently propelled across the arc. 

If an open arcing technique is attempted much below the threshold current level, the low arcing forces will not be sufficient to prevent large drops from forming at the wire tip. These droplets move erratically across the arc under normal gravity. 

Short Circuit Welding Settings

Short circuit welding, also known as short arc or dip transfer welding, typically uses lower welding amperage and voltage settings compared to other welding techniques.

Related reading: Metal Transfer Mode in GMAW, FCAW & SMAW Welding

Short circuit welding is a type of gas metal arc welding (GMAW) also known as MIG welding.

The settings for short circuit welding depend on several factors, including the material being welded, the thickness of the material, and the welding position. However, there are some general guidelines that can be followed.

  1. Voltage: The voltage setting is usually less than 22 volts. Lower voltages are used for thinner materials and higher voltages for thicker materials.
  2. Wire Feed Speed: The wire feed speed is typically between 80 and 300 inches per minute (ipm). Lower wire feed speeds are used for thinner materials and higher wire feed speeds for thicker materials.
  3. Amperage: The amperage setting depends on the thickness of the material being welded. For thin materials, the amperage should be set lower, around 50-150 amps. For thicker materials, the amperage should be set higher, around 150-250 amps.
  4. Gas Flow Rate: The gas flow rate should be set between 20-30 cubic feet per hour (cfh).
See also  Who is a Coded welder?

The welding amperage for short circuit welding is generally less than 200 amps for 0.9 mm diameter wire, and the voltage is also relatively low.

short-circuit-transfer

The type of shielding gas used in short circuit welding depends on the material being welded.

For carbon-manganese steels, carbon dioxide (CO2) or a mixture of 75% argon and 25% CO2 is commonly used.

Why is Short Circuit Transfer not permitted on pressure vessels, Bridges, and Navel vessels?

Short circuit welding, also known as short arc or dip transfer welding, is best suited for thin ferrous materials and root passes of thicker steels due to its low welding current and voltage.

However, it can be challenging to use the short circuiting mode for thicker materials because of the small wire diameters (1.2 mm or smaller) and low currents (less than 200 A for 0.9 mm diameter wire), which result in a low heat input that can cause fusion problems.

For this reason, welding specifications for critical structural applications such as pressure vessels, bridges, and naval vessels prohibit the use of short circuit transfer mode when the GMAW process is employed.

Carbon dioxide (CO2) or 75% argon – 25% CO2 are the typical shielding gases used for carbon-manganese steels.

Application of Short Circuit Transfer

Since only a small amount of heat is generated with a Short Circuit Transfer mode in welding, this only leads to a lower melting rate. 

In some applications, however, this is the best choice! A Short Circuit Transfer or a short arc is used, for example, with thin sheets up to a thickness of 3 mm

See also  ER308LSi vs ER309LSi vs 316LSi

The short arc is ignited by a deliberately created short circuit mode. It is recommended for root run welding and out-of-position welding positions when you do not want the molten metal to flow down with gravity. 

The material transfer results in coarse droplets when using short-circuit welding mode.

Advantages of Short Circuit Welding

Short Circuit Welding offers several advantages over other welding techniques, such as:

  1. Lower heat input: Short circuit transfer results in lower heat input to the base metal, which is beneficial for preventing distortion and minimizing the risk of burn-through.
  2. Lower spatter: Since the welding wire does not stay in the molten state for long periods of time, there is less spatter produced during welding.
  3. Better control: Short circuit transfer allows for better control over the welding process, making it easier to achieve a consistent and uniform weld bead.