This sheet metal gauge calculator converts a gauge number to thickness in inches and millimetres for carbon steel, galvanized steel, stainless steel, aluminium, copper and brass, plus the British SWG and the BWG used for tube walls. It also works the other way, finding the nearest gauge for a thickness. You also get the sheet weight for standard sheet sizes and a rule-of-thumb welding starting point for thin sheet. The same gauge number means a different thickness in each system: 16 gauge is 1.52 mm in steel, 1.59 mm in stainless and 1.29 mm in aluminium.
Quick answer
Sheet gauge to thickness calculator
Sheet size for weight
Animated: a slotted gauge disc turns to the gauge you picked.
Animated: the same gauge number in each system, drawn to scale.
Thicknesses are nominal. Mill tolerances (for example ASTM A568 for carbon steel sheet and A480 for stainless) allow the actual thickness to vary, so measure with a micrometer when it matters. Weight uses the density shown; a G90 (Z275) zinc coating adds about 0.28 kg/m² to galvanized sheet.
What sheet metal gauge means
Gauge numbers come from old wire-drawing practice: each pass through a die made the wire thinner, so a higher gauge number means thinner material. The numbers are not linked to any unit, and each gauge system has its own steps:
- Manufacturers’ Standard Gauge (steel): for uncoated carbon steel sheet. It was based on weight, at 41.82 lb/ft² per inch of thickness, so 16 gauge was defined as 2.5 lb/ft² = 0.0598″.
- Galvanized steel gauge: the steel gauge plus the zinc coating, about 0.0037″ thicker at each gauge.
- Stainless steel gauge: usually follows the older US Standard Gauge, so 16 gauge is 1/16″ (0.0625″) and 11 gauge is 1/8″.
- Brown & Sharpe (AWG): used for aluminium, copper and brass sheet, and for electrical wire. Each gauge is about 11% thinner than the one before.
- SWG (Imperial Standard Wire Gauge): still used for sheet and wire in the UK, India, Australia and other countries.
- BWG (Birmingham Wire Gauge): used for the wall thickness of heat-exchanger, boiler and instrument tubing.
Animated: thickness against gauge number for each system. Dots mark the selected gauge.
Sheet metal gauge chart
| Gauge | Steel (in) | Steel (mm) | Galvanized (mm) | Stainless (in) | Stainless (mm) | Aluminium (in) | Aluminium (mm) |
|---|---|---|---|---|---|---|---|
| 7 | 0.1793 | 4.55 | – | 0.1875 | 4.76 | 0.1443 | 3.67 |
| 8 | 0.1644 | 4.18 | 4.27 | 0.1719 | 4.37 | 0.1285 | 3.26 |
| 9 | 0.1495 | 3.80 | 3.89 | 0.1563 | 3.97 | 0.1144 | 2.91 |
| 10 | 0.1345 | 3.42 | 3.51 | 0.1406 | 3.57 | 0.1019 | 2.59 |
| 11 | 0.1196 | 3.04 | 3.13 | 0.1250 | 3.17 | 0.0907 | 2.30 |
| 12 | 0.1046 | 2.66 | 2.75 | 0.1094 | 2.78 | 0.0808 | 2.05 |
| 13 | 0.0897 | 2.28 | 2.37 | 0.0938 | 2.38 | 0.0720 | 1.83 |
| 14 | 0.0747 | 1.90 | 1.99 | 0.0781 | 1.98 | 0.0641 | 1.63 |
| 15 | 0.0673 | 1.71 | 1.80 | 0.0703 | 1.79 | 0.0571 | 1.45 |
| 16 | 0.0598 | 1.52 | 1.61 | 0.0625 | 1.59 | 0.0508 | 1.29 |
| 17 | 0.0538 | 1.37 | 1.46 | 0.0563 | 1.43 | 0.0453 | 1.15 |
| 18 | 0.0478 | 1.21 | 1.31 | 0.0500 | 1.27 | 0.0403 | 1.02 |
| 19 | 0.0418 | 1.06 | 1.16 | 0.0438 | 1.11 | 0.0359 | 0.91 |
| 20 | 0.0359 | 0.91 | 1.01 | 0.0375 | 0.95 | 0.0320 | 0.81 |
| 21 | 0.0329 | 0.84 | 0.93 | 0.0344 | 0.87 | 0.0285 | 0.72 |
| 22 | 0.0299 | 0.76 | 0.85 | 0.0313 | 0.80 | 0.0253 | 0.64 |
| 23 | 0.0269 | 0.68 | 0.78 | 0.0281 | 0.71 | 0.0226 | 0.57 |
| 24 | 0.0239 | 0.61 | 0.70 | 0.0250 | 0.64 | 0.0201 | 0.51 |
| 25 | 0.0209 | 0.53 | 0.63 | 0.0219 | 0.56 | 0.0179 | 0.45 |
| 26 | 0.0179 | 0.45 | 0.55 | 0.0188 | 0.48 | 0.0159 | 0.40 |
| 27 | 0.0164 | 0.42 | 0.51 | 0.0172 | 0.44 | 0.0142 | 0.36 |
| 28 | 0.0149 | 0.38 | 0.47 | 0.0156 | 0.40 | 0.0126 | 0.32 |
| 29 | 0.0135 | 0.34 | 0.44 | 0.0141 | 0.36 | 0.0113 | 0.29 |
| 30 | 0.0120 | 0.30 | 0.40 | 0.0125 | 0.32 | 0.0100 | 0.25 |
SWG and BWG gauge chart
| Gauge | SWG (in) | SWG (mm) | BWG (in) | BWG (mm) |
|---|---|---|---|---|
| 3 | 0.252 | 6.40 | 0.259 | 6.58 |
| 4 | 0.232 | 5.89 | 0.238 | 6.05 |
| 5 | 0.212 | 5.38 | 0.22 | 5.59 |
| 6 | 0.192 | 4.88 | 0.203 | 5.16 |
| 7 | 0.176 | 4.47 | 0.18 | 4.57 |
| 8 | 0.16 | 4.06 | 0.165 | 4.19 |
| 9 | 0.144 | 3.66 | 0.148 | 3.76 |
| 10 | 0.128 | 3.25 | 0.134 | 3.40 |
| 11 | 0.116 | 2.95 | 0.12 | 3.05 |
| 12 | 0.104 | 2.64 | 0.109 | 2.77 |
| 13 | 0.092 | 2.34 | 0.095 | 2.41 |
| 14 | 0.08 | 2.03 | 0.083 | 2.11 |
| 15 | 0.072 | 1.83 | 0.072 | 1.83 |
| 16 | 0.064 | 1.63 | 0.065 | 1.65 |
| 17 | 0.056 | 1.42 | 0.058 | 1.47 |
| 18 | 0.048 | 1.22 | 0.049 | 1.24 |
| 19 | 0.04 | 1.02 | 0.042 | 1.07 |
| 20 | 0.036 | 0.91 | 0.035 | 0.89 |
| 21 | 0.032 | 0.81 | 0.032 | 0.81 |
| 22 | 0.028 | 0.71 | 0.028 | 0.71 |
| 23 | 0.024 | 0.61 | 0.025 | 0.64 |
| 24 | 0.022 | 0.56 | 0.022 | 0.56 |
| 25 | 0.02 | 0.51 | 0.02 | 0.51 |
| 26 | 0.018 | 0.46 | 0.018 | 0.46 |
| 27 | 0.0164 | 0.42 | 0.016 | 0.41 |
| 28 | 0.0148 | 0.38 | 0.014 | 0.36 |
| 29 | 0.0136 | 0.35 | 0.013 | 0.33 |
| 30 | 0.0124 | 0.31 | 0.012 | 0.30 |
Steel sheet weight by gauge
Weights below use 7.85 g/cm³ (0.2836 lb/in³) and the nominal thickness. Older Manufacturers’ Standard Gauge tables list slightly higher weights (for example 2.50 lb/ft² for 16 gauge) because that gauge was defined at 41.82 lb/ft² per inch.
| Steel gauge | Thickness (mm) | kg/m² | lb/ft² | 4 × 8 ft sheet (lb) | 1250 × 2500 mm sheet (kg) |
|---|---|---|---|---|---|
| 10 | 3.42 | 26.82 | 5.49 | 175.8 | 83.8 |
| 11 | 3.04 | 23.85 | 4.88 | 156.3 | 74.5 |
| 12 | 2.66 | 20.86 | 4.27 | 136.7 | 65.2 |
| 14 | 1.90 | 14.89 | 3.05 | 97.6 | 46.5 |
| 16 | 1.52 | 11.92 | 2.44 | 78.1 | 37.3 |
| 18 | 1.21 | 9.53 | 1.95 | 62.5 | 29.8 |
| 20 | 0.91 | 7.16 | 1.47 | 46.9 | 22.4 |
| 22 | 0.76 | 5.96 | 1.22 | 39.1 | 18.6 |
| 24 | 0.61 | 4.77 | 0.98 | 31.2 | 14.9 |
| 26 | 0.45 | 3.57 | 0.73 | 23.4 | 11.2 |
| 28 | 0.38 | 2.97 | 0.61 | 19.5 | 9.3 |
Thickness to gauge finder
Find the nearest gauge
Welding thin sheet by gauge
The calculator shows a starting point based on two common rules of thumb: about 1 amp for every 0.001″ (0.025 mm) of thickness for steel with MIG or TIG, and a wire or tungsten size that suits the thickness. Aluminium usually needs about 25–50% more current because of its high thermal conductivity. Always run test welds and follow the welding machine chart or the WPS.
| Steel gauge | mm | MIG wire | Approx. amps | Notes |
|---|---|---|---|---|
| 24–20 | 0.6–0.9 | 0.6 mm (0.023″) | 25–40 | Stitch or skip weld; TIG or pulsed MIG preferred; risk of burn-through |
| 18–16 | 1.2–1.5 | 0.6–0.8 mm | 45–60 | Short circuit transfer, Ar/CO₂ gas; use copper backing on butt joints |
| 14–12 | 1.9–2.7 | 0.8 mm (0.030″) | 75–105 | Single pass on most joints |
| 11–10 | 3.0–3.4 | 0.8–0.9 mm | 120–135 | Square butt with a small gap, or bevel for full penetration |
Tips for specifying sheet thickness
- Specify in mm or inches on drawings and purchase orders. Gauge alone can be misread, especially between steel, stainless and aluminium.
- Name the gauge system if you do use gauge, for example “16 ga (0.0598″) carbon steel, MSG”.
- Check tolerances: thin sheet can be supplied noticeably under nominal and still meet the standard.
- Galvanized sheet gauge includes the zinc; the steel core is thinner.
- Tube walls are usually given in BWG (for example 16 BWG = 1.65 mm) or as a minimum wall rather than an average wall.
Frequently asked questions
How thick is 16 gauge sheet metal?
Why does a higher gauge number mean thinner metal?
Is aluminium gauge the same as steel gauge?
What gauge is 3 mm steel?
What is the difference between SWG and BWG?
Summary
Sheet gauge numbers are not universal: carbon steel uses the Manufacturers’ Standard Gauge, galvanized steel adds the zinc coating, stainless steel follows the older US Standard Gauge, aluminium, copper and brass use Brown & Sharpe, and the UK uses SWG. Higher numbers are thinner. Use the calculator to convert gauge to mm or inches, find the nearest gauge for a thickness, and estimate sheet weight. On drawings, state the thickness in mm or inches to avoid mistakes.